Insight · Dimensional stability

Moisture absorption and dimensional change in nylon

8 November 2026 · Himing New Material (Zhongshan CSII) Co., Ltd.

The short answer: most dimensional problems on nylon parts are not moulding faults but a mismatch between the state the part is inspected in and the state it was designed for. PA6 and PA66 take up moisture from the air, swell and lose stiffness; glass fibre dilutes the uptake without removing it. Decide first how humid the part will live and in which state it is measured, then cut the tool using that grade's measured moisture-expansion coefficient.

1. What moisture changes

PropertyDryConditionedNote
Tensile strengthBaseline (100%)Down 15–40%PA6 usually loses more than PA66; worse at temperature
Flexural modulusBaseline (100%)Down 20–50%Stiffness loss exceeds strength loss; thin parts feel soft
Notched impactBaselineRisesWater plasticises — tougher but less stiff
DimensionsBaseline0.3–1.0% linearDepends on grade and glass content; calculate from measured coefficients
ElectricalBaselineInsulation fallsAssess CTI and volume resistivity in the hot-wet state

Ranges are industry-typical and vary with grade, glass content, temperature and humidity; design values must come from the grade's measured data.

2. Estimating the dimensional increment

Three steps, rather than a single universal percentage:

  1. Establish the equilibrium moisture content at the service environment (temperature, humidity, wall thickness).
  2. Convert with the grade's moisture-expansion coefficient — the linear growth per 1% moisture.
  3. Apply the increment separately along and across the flow; glass-filled systems differ substantially between the two.

If a supplier gives water uptake but not an expansion coefficient, estimate from a similar system — but measure the critical conditioned dimensions on the first tool and correct before production. Skipping this step guarantees a dimensional fight later.

3. What each control actually does

Drying: controls moisture before moulding to prevent degradation and voids; it does not change what happens to the finished part.

Conditioning: brings parts close to service equilibrium before shipping, stabilising dimensions and properties early. Suits precision parts, but costs time and space and needs a defined conditioning spec.

Annealing: relieves stress and stabilises crystallinity, reducing later distortion and cracking; it does not stop absorption, only makes the drift more predictable.

4. Three common misjudgements

  1. Using dry dimensions as assembly dimensions. A part straight off the machine is the driest and smallest it will ever be; design to that and assembly runs tight.
  2. Ignoring ambient humidity. Equilibrium moisture differs between a wet coastal summer and a dry northern winter; the same tool behaves differently in two plants.
  3. Assuming glass stops absorption. The matrix still absorbs, and anisotropy grows — long thin parts bend more, not less.

5. Questions engineers ask

How far apart are dry and conditioned dimensions?+
It depends on grade, glass content and ambient humidity, so there is no universal number. PA6 equilibrates at a higher moisture content than PA66, and unreinforced systems are more sensitive than glass-filled ones. The engineering method: equilibrium moisture at the service environment times the grade moisture-expansion coefficient, then cut the tool by that per-side increment. Request both numbers as measured data — do not substitute industry rules of thumb.
Should the mould be cut to the dry or the wet state?+
To the state the part is actually in when it matters. Most structural parts have absorbed close to equilibrium by assembly, so cavity dimensions follow the conditioned state. If a part is assembled dry and absorbs later, assess the clearance change instead. Before deciding, agree on the state in which dimensions are inspected.
Does annealing solve dimensional problems?+
Annealing relieves internal stress and stabilises crystallinity, which reduces later distortion, but it does not change moisture equilibrium. An annealed part still absorbs moisture and grows; it just drifts more predictably. Treat annealing as stress relief, not as moisture protection.
Does glass fibre stop moisture absorption?+
No. Glass does not absorb water, but the matrix still does; glass only dilutes the uptake by volume. GF30 absorbs roughly seventy percent of an unreinforced system, while anisotropy increases — less expansion along the flow, more across it, so long thin parts bend more.

Related: moisture sensitivity is itself one of the criteria when choosing between PA6 and PA66.