Selection guide · 01

PA6+GF30 vs PA66+GF30: choose by heat, moisture and impact

The short answer: above 120 °C continuous, or where HDT must exceed 220 °C, use PA66+GF30. For room-temperature structural parts where impact and cost matter most, PA6+GF30 is the better fit. For wet environments or tight dimensional tolerance, prefer PA66. At the same 30% glass loading the flexural moduli are close — the real dividing line is heat resistance and moisture uptake.

Himing New Material (Zhongshan CSII) Co., Ltd. · IATF 16949 · ISO 9001 · CRCC · Zhongshan, Guangdong

1. The real difference at equal glass loading

Typical ranges at the GF30 level, for first-pass screening. Final selection follows the data sheet of the specific grade.

PropertyPA6+GF30PA66+GF30What it means for selection
Melting point~220 °C~255 °CPA66 runs a 30–40 °C higher processing window
HDT @ 1.8 MPa~195–210 °C~240–250 °CSets the continuous-temperature ceiling
Water absorption, 24 h1.6–2.0%1.0–1.3%PA6 shifts more in dimension and strength after conditioning
Tensile strength, dry120–160 MPa150–190 MPaPA66 is usually higher at equal glass loading
Flexural modulus7,500–9,000 MPa7,000–8,700 MPaClose; fibre length and dispersion matter more than the base resin
Notched impact, 23 °C8–12 kJ/m²10–15 kJ/m²Grade-specific toughening dominates — check the data sheet
Processing temperature240–270 °C270–300 °CPA66 asks more of the machine and the mould temperature
Cost index100115–125Rough index at equal glass content and FR rating

General material ranges for screening. Measured values for Himing grades are on each product page. Contractual acceptance follows the TDS and batch COA.

2. A three-step decision

Step 1 · Heat

Continuous service above 120 °C, or peaks near 150 °C → PA66. Below 100 °C with only brief excursions → PA6 can be evaluated.

Step 2 · Moisture and tolerance

High humidity, water contact or tight fits → PA66. Dry environment and loose tolerance → PA6's higher uptake is not a problem.

Step 3 · Impact and cost

Room-temperature impact, cost-sensitive, non-cosmetic → PA6. If both pass, compare total annual cost, not the per-kilo price.

3. Three common mistakes

  1. Comparing dry tensile strength only. PA6 loses more strength and modulus after moisture conditioning than PA66. Ask for conditioned data, not just the dry-as-moulded sheet.
  2. Assuming more glass is safer. GF35/GF40 buys modulus at the cost of impact, flow and surface finish; thin walls show fibre read-through and weaker weld lines. Fix glass content from wall thickness and flow length first.
  3. Estimating an FR grade from its base grade. The flame-retardant package changes toughness. Use the measured notched impact of the FR grade itself.

4. The Himing grades this maps to

Measured typical values; full properties and test conditions are on each product page.

GradeTensile MPaFlex modulus MPaNotched impact kJ/m²Typical use
PA6 + 30% GF, FR V-01238,6009FR structures, electrical housings
PA66 + 30% GF, structural1557,20014Under-hood brackets, end caps
PA66 + 35% GF, heavy-duty1918,71321Rail fastenings, heavy structures

5. Questions buyers ask

Can PA6+GF30 replace PA66+GF30 directly?+
For many room-temperature, short-cycle parts, yes — but check two things first. Continuous service above 120 °C: PA6 HDT is around 200 °C versus 245 °C for PA66. And moisture: PA6 absorbs more water, so dimensions and properties shift further after conditioning. Send the part, wall thickness, load and service life and we will benchmark both under the same conditions.
Is a higher glass content always better?+
No. Going from GF30 to GF35/GF40 raises flexural modulus and tensile strength but reduces notched impact, flow length and surface quality, with more fibre read-through. Thin walls with long flow paths are usually better at GF20–GF30; only sustained-load, low-creep parts justify GF35 and above.
How much does V-0 flame retardancy cost in toughness?+
It depends on the FR system and loading. A halogen-free phosphorus–nitrogen package typically affects notched impact less than a halogenated one. Always use the measured impact value of the FR grade itself — never estimate it from the non-FR base grade.
How do I judge whether a Chinese grade can replace an imported one?+
Compare four things on the same test standard and conditions: dry-as-moulded tensile and flexural modulus, notched impact including low temperature, HDT, and property retention after ageing or moisture conditioning. Comparing dry tensile strength alone is the most common source of a bad substitution.

Send us the part and the current grade

A grade recommendation within 24 hours; samples from 500 kg in 7–10 days.